{"operation":"document","citation":"P-98-007","title":"NTSB Safety Recommendation P-98-007","source_type":"guidance","agency":"National Transportation Safety Board","status":"guidance","official":true,"published_on":"1998-04-30","effective_on":"1998-04-30","summary":"THE NTSB RECOMMENDS THAT THE PLASTICS PIPE INSTITUTE: ADVISE YOUR MEMBERS TO NOTIFY PIPELINE SYSTEM OPERATORS IF ANY OF THEIR PIPING PRODUCTS, OR MATERIALS USED IN THE MANUFACTURE OF PIPING PRODUCTS, CURRENTLY IN SERVICE FOR NATURAL GAS OR OTHER HAZARDOUS MATERIALS INDICATE POOR RESISTANCE TO BRITTLE-LIKE FAILURE.","machine_formats":{"json":"https://regulus.evalyn.ai/document/ntsb-recommendation-p-98-007.json","markdown":"https://regulus.evalyn.ai/document/ntsb-recommendation-p-98-007.md"},"app_url":"https://regulus.evalyn.ai/document/ntsb-recommendation-p-98-007","source_url":"https://data.ntsb.gov/carol-main-public/sr-details/P-98-007","body":"NTSB safety recommendation P-98-007.\n\nTHE NTSB RECOMMENDS THAT THE PLASTICS PIPE INSTITUTE: ADVISE YOUR MEMBERS TO NOTIFY PIPELINE SYSTEM OPERATORS IF ANY OF THEIR PIPING PRODUCTS, OR MATERIALS USED IN THE MANUFACTURE OF PIPING PRODUCTS, CURRENTLY IN SERVICE FOR NATURAL GAS OR OTHER HAZARDOUS MATERIALS INDICATE POOR RESISTANCE TO BRITTLE-LIKE FAILURE.\n\nPriority: CLASS II\n\nOverall Status: Closed - Acceptable Action\n\nIssued Date: 1998-04-30\n\nAdopted Date: 1998-04-23\n\nOverall Date Closed: 1998-10-19\n\nSynopsis: DESPITE THE GENERAL ACCEPTANCE OF PLASTIC PIPING AS A SAFE & ECONOMICAL ALTERNATIVE TO PIPING MADE OF STEEL OR OTHER MATERIALS, THE BOARD NOTES THAT A NUMBER OF PIPELINE ACCIDENTS IT HAS INVESTIGATED HAVE INVOLVED PLASTIC PIPING THAT CRACKED IN A BRITTLE-LIKE MANNER. FOR EXAMPLE, ON 10/17/94, AN EXPLOSION & FIRE IN WATERLOO, IOWA, DESTROYED A BUILDING & DAMAGED OTHER PROPERTY. SIX PERSONS DIED & SEVEN WERE INJURED IN THE ACCIDENT. THE BOARD INVESTIGATION DETERMINED THAT NATURAL GAS HAS BEEN RELEASED FROM A PLASTIC SERVICE PIPE THAT HAD FAILED IN A BRITTLE-LIKE MANNER AT A CONNECTION TO A STEEL MAIN.\n\nProbable Cause: None\n\nNtsbnumber: DCA95MP001\n\nReport Number: SIR-98-01\n\nAddressee Name: Plastics Pipe Institute\n\nAddressee Status: Closed - Acceptable Action\n\nAddressee Date Closed: 1998-10-19\n\nAddressee Acronym: PPI\n\nAddressee Organization Type: A-Associations\n\nCommunication Date: 1998-06-30\n\nCommunication Type: Official Correspondence\n\nCommunication Contents: (Letter Mail Controlled 7/9/98 2:51:30 PM MC# 980864) BY COPY OF YOUR ABOVE SUBJECT LETTER TO EACH FUEL GAS DIVISION MEMBER COMPANY WE ADVISED OUR MEMBERS TO NOTIFY THEIR CUSTOMERS OF ANY OF THEIR MATERIALS WITH \"POOR RESISTANCE TO BRITTLE-LIKE FAILURE\"AS RECOMMENDED.\n\nAddressee Acronym: PPI\n\nAddressee Organization Type: A-Associations\n\nCommunication Date: 1998-10-19\n\nCommunication Type: Official Correspondence\n\nCommunication Contents: THE SCOPE BOARD'S REPORT WAS LIMITED TO FIELD BENDS FOR UNCASED DIRECT BURIAL APPLICATIONS. THE REPORT NOTED THAT PLASTIC PIPING IS OFTEN DELIVERED TO JOB SITES IN BANDED COILS SOME RESIDUAL BENDING IN THE PIPING REMAINS AFTER THE BANDS ARE REMOVED. THE REPORT STATED THAT THE \"GAS INDUSTRY FIELD (EMPHASIS ADDED) BEND RESIDUAL RECOMMENDATIONS DO NOT ADDRESS RESIDUAL COIL BENDING P-98-9 WAS ISSUED TO THE PPI TO ENCOURAGE THE PLASTIC PIPING MANUFACTURERS TO REVISE THEIR PIPELINE BEND RADIUS RECOMMENDATIONS TO TAKE INTO ACCOUNT THE EFFECTS OF RESIDUAL COIL BENDS INPLASTIC PIPING. THE BOARD UNDERSTANDS THAT SOME GAS SYSTEM OPERATORS ARE AWARE OF OLDER PLASTIC PIPING MATERIALS HAVING A SUSCEPTIBILITY TO PREMATURE BRITTLE-LIKE CRACKING & ARE MONITORING THEIR PLASTIC PIPELINE SYSTEMS. THE BOARD'S REPORT CONCLUDED THAT THE GAS PIPELINE SYSTEM OPERATORS HAVE HAD INSUFFICIENT NOTIFICATION THAT MUCH OF THE PLASTIC PIPE MANUFACTURED FROM THE 1960S THROUGH THE MID-1980S MAY BE SUSCEPTIBLE TO BRITTLE-LIKE CRACKING &, THEREFORE, MAY NOT HAVE IMPLEMENTED ADEQUATE PIPELINE SURVEILLANCE & REPLACEMENT PROGRAMS FOR THEIR OLDER PIPING. AS THE BOARD'S REPORT NOTES, PLASTIC PIPE'S ECONOMY, OUTSTANDING CORROSION RESISTANCE, LIGHT WEIGHT, EASE OF INSTALLING & JOINING, & DUCTILITY HAVE ALL CONTRIBUTED TO MAKE PLASTIC PIPING THE MATERIAL OF CHOICE FOR NATURAL GAS DISTRIBUTION SYSTEMS. THE BOARD DOES NOT PROPOSE TO DISCOURGE PIPELINE SYSTEM OPERATORS FROM USING PLASTIC PIPE; HOWEVER, THIS IMPORTANT ISSUE NEEDS THE ATTENTION OF ALL GAS PIPELINE OPERATORS HAVING OLDER PLASTIC PIPING IN SERVICE. BECAUSE THE PPI PROVIDED COPIES OF THE BOARD'S 4/30/98, LETTER & ADVISED ITS MEMBERS AS REQUESTED, P-98-7 THROUGH -9 HAVE BEEN CLASSIFIED \"CLOSED--ACCEPTABLE ACTION.\"","truncated":false,"body_characters":3682}